How to Make Limewash Paint: Ratios, Coats, and Fixes

This post contains affiliate links. As an Amazon Associate, we earn from qualifying purchases.

To make limewash paint, mix hydrated lime or lime putty with water to roughly 15 to 20 percent lime solids by weight. The National Lime Association’s working ratio is a 50 lb bag of hydrated lime to 30.5 gallons of water for a 20:80 mix, or 40.5 gallons for a thinner 15:85 batch.

That weight figure is where the two main schools of thought split. The National Lime Association publishes exact ratios down to the gallon. The NSW Heritage Council’s technical bulletin says to mix by eye instead, because each batch of lime takes a different amount of water. Both are chasing the same target: something the consistency of thin cream. For a practical walkthrough, see this guide on how to make limewash paint.

What follows is the practical route through both positions. Three starting materials, the application sequence that gets a coat to actually bond, the surfaces that will reject limewash outright, and the specific reasons a finished wall goes chalky or crazes.

Key Takeaways

  • Mix to 15 to 20 percent lime solids by weight. A 50 lb bag of hydrated lime plus 30.5 gallons of water hits 20:80. The same bag plus 40.5 gallons hits 15:85.
  • Thin coats only. Limewash goes on semi-transparent and dries opaque. A visible thick layer will craze and crack, especially down in the recesses of rough masonry.
  • Dampen the wall before every coat. Fast drying disrupts carbonation and leaves a weak, cohesionless finish that cracks and powders.
  • Plan on three or four coats minimum. SPAB calls for at least three or four. The National Park Service recommends three or more for a first limewashing, with drying times of 24 hours or longer depending on conditions.
  • Skip acrylic “limewash” paint if breathability is the reason you’re here. NSW states plainly that these products do not transmit moisture and salts the way traditional limewash does.

What Ratio Actually Makes Limewash Paint?

Fifteen to twenty percent lime solids, by weight, is the number to hold in your head. The National Lime Association’s technical brief on limewash for masonry and stucco works it out in gallons so you don’t have to: 50 lb of hydrated lime into 30.5 gallons of water for the 20:80 end, or 40.5 gallons for the thinner 15:85 end.

A 50 lb bag of hydrated lime mixed with 30.5 gallons of water yields approximately a 20:80 lime-to-water ratio by weight. The same bag with 40.5 gallons of water yields a thinner 15:85 mix. Lime putty runs about 50 percent water, so 100 pounds of putty plus roughly 24 gallons of water reaches the same 20:80 target.

The putty math is the part of how to make limewash paint that catches people. Because putty is roughly half water already, the water inside it displaces about 6.1 gallons of what you’d otherwise add. Skip that correction and you’ll mix a batch that’s noticeably too thick.

Quicklime is a third route and the one I’d steer most readers away from. To slake it you add water at roughly 8 gallons to 38 pounds of quicklime. The reaction is exothermic and the resulting hydroxide is highly basic enough to cause chemical burns to skin, eyes and tissue. ASTM C 5-03 covers quicklime for structural purposes if you want the formal spec, but the safety case is the real argument.

Mixing by Weight vs Mixing by Eye: Where the Sources Split

You can follow a published how to make limewash paint ratio to the gallon and still get a bad batch. The NSW Heritage Council’s NSW heritage limewash maintenance guide says mixing should generally be done by eye rather than by weight, since each lime takes a different amount of water. Their target is thin cream, generally around 15 to 20 percent lime.

Both are right, and the disagreement is smaller than it looks. Weight gets you into the range. Eye gets you to the finish, because the lime you bought last year and the lime you bought this week will not wet out identically.

Here’s where the authorities genuinely diverge, and you should know which position you’re following before you start:

Question One position The other position
Mixing method National Lime Association: 15 to 20% lime, 80 to 85% water by weight NSW Heritage Council: mix by eye, each lime takes different water
Renewal interval SPAB: renew every five years National Park Service: annual reapplication to counter weathering
Additives NSW Heritage Council: an egg-cupful of raw linseed oil optional SPAB: linseed and tallow reduce breathability; tallow may support mould
Pigment timing NSW and SPAB: final layers, or just the last coat or two National Park Service: pigments added in moderation, not limited to final coats
Bagged hydrated lime lime.org and NSW: bagged recipes given as standard SPAB: putty from ordinary bagged lime can give inferior limewash

That last row matters more than the rest. SPAB’s limewash guidance warns that preparing putty from ordinary non-hydraulic bagged lime can result in inferior limewash, while the National Lime Association and NSW both hand you bagged-lime recipes as the normal route. If you’re working on old masonry and you only get one shot, buy putty.

Three Starting Materials and What Each One Asks of You

Hydrated lime is the cheapest and most available. Lime putty is the most forgiving. Quicklime is the most dangerous and the least necessary for a first batch.

Hydrated Lime From a Bag

Sold at builders’ merchants as bag lime. NSW gives it a standard recipe: mix water into the lime gradually, beating well to get as thorough a mix as possible. The catch is that bagged lime can produce a wash with weaker adhesion, which SPAB attributes to the starting material itself rather than your technique.

Lime Putty

Thicker, wetter, and about half water by weight. NSW’s method is a few trowelfuls of putty in a bucket, covered with about 75 mm of water, worked to a smooth paste, then thinned toward cream. You get more control over the final consistency because you’re adding water in visible increments instead of trying to wet down a dry powder.

Quicklime

Calcium oxide, CaO. It must be kept dry in storage and it combines with water violently, producing great heat and spitting that will burn. It is generally only available to tradespeople with a demonstrated need. Slaking it on site is how limewash was made for centuries and how almost nobody should make it now.

I’ll be honest about my own bias here. I came to this from pigment and binder experiments, mixing small test batches of egg tempera and milk paint just to understand what paint actually is. Limewash fits that same curiosity, and the lesson I keep relearning is that a few ingredients and some practice teach you more than a big kit ever will. (I ruined a batch early on by adding water to the powder too fast and getting a lumpy slurry I had to sieve twice.)

The Application Sequence That Actually Bonds

Before you start: Lime is caustic. Wear waterproof clothing, gloves, barrier cream and goggles, and keep an eye bath or spray bottle of clean lukewarm water within reach. If limewash gets into your eyes, rinse continuously for 20 minutes and seek medical assistance. Quicklime is worse: keep it dry, and never lean over the bucket while it slakes.

  1. Brush the wall down first. Remove loose dirt and treat minor mould growth with fungicide. Skip this and your coat bonds to dust, which is exactly as durable as it sounds.
  2. Dampen the surface. A hand-pumped spray is the standard tool. The National Park Service’s National Park Service limewash course is blunt about the consequence: if the limewash dries too quickly, carbonation is disrupted and you get a weak, cohesionless finish that cracks and powders.
  3. Load a large, rough-textured brush. The National Lime Association does not recommend sprayers, because it’s hard to work the limewash into the substrate and the work has to be gone over again with a brush anyway. If you insist on a sprayer, pre-screen the mix to avoid plugging the nozzle.
  4. Apply thin and work it in. Keep a wet edge the whole time. Thin layers build a conformal coat; a visible thick layer crazes on drying.
  5. Wait 24 hours or longer. Drying time depends on humidity and temperature. This is the step that wrecks weekend plans. A four-coat job takes several days, not an afternoon.
  6. Dampen again and repeat. Each preceding coat should be allowed to dry and the surface dampened down before the next goes on.
  7. Build to three or four coats. Successive limewashings later in the wall’s life will need fewer layers, which is the one piece of good news in the whole process.

The mix should pour like thin cream. If it sits up on the brush instead of flowing off it, add water.

Which Surfaces Take Limewash and Which Reject It

limewash paint on limestone versus impervious flint surface test

Flint and hard brick will not take limewash, full stop. They’re impervious, and an impervious substrate gives the wash nothing to grip or breathe through.

The suitable list is longer than most people expect. Lime plaster and render, earth walls, limestone, timber and most old limewash all work. Smooth surfaces like hard-trowelled render, dense stone, rusted steel and glass can be limewashed, but they benefit from a roughening-up with fine-to-medium abrasives, steel wool or wire brushing first.

What to avoid:

  • Flint and hard brick. Impervious, so the coat has nothing to bond to.
  • Sandstone, on a first limewashing. SPAB calls first-time limewashing inadvisable here.
  • Cement render, plasterboard and emulsion. Limewash takes less well to all three, though it may be possible if the mix is modified for better adhesion.
  • Anything previously sealed. Old walls should never be coated with water repellents or other sealing products, because the coating traps moisture and causes damage.

If you’re planning to whitewash brick rather than limewash it, check the brick type first. A hard, dense brick is the wrong candidate for either finish. The limewash pros and cons come down to breathability on one side and renewal frequency on the other, and on a sealed wall you lose the breathability argument entirely.

What most people get wrong: Sealing an old wall first “to protect it.” The coating traps moisture behind an impermeable film, and the damage shows up as blown plaster and salt bloom within a couple of seasons.

Why Your Limewash Crazed, Powdered, or Brushed Off

Limewash wall showing crazing and chalky powder failure

You brushed on what looked like a solid coat, it dried patchy and pale, and now it rubs off on your sleeve. That’s the most common outcome and it almost always traces to one of four causes.

Symptom Likely cause Fix
Crazed, cracked in recesses Mix too thick Thin toward 15 to 20% solids and add water
Powdery, chalky, rubs off Dried too fast, carbonation disrupted Dampen first; work in spring or fall, out of sun and wind
Brushed off on clothes Poor adhesion from thick coats or no dampening Re-prep the wall, apply thinner, dampen between coats
Patchy, uneven colour Batch-to-batch mismatch Mix enough for a full coat at once and agitate throughout

SPAB lists the adhesion failures explicitly: preparation with ordinary bagged lime, coats applied excessively thickly, inadequate dampening down, or too rapid drying out. Notice that three of those four are technique, not product.

The NPS durability of traditional limewashes study adjusted its test recipes to a viscosity of 17 seconds at 70 degrees in a #4 Ford cup, with some recipes at 12 seconds. That’s a useful sanity check if you’re mixing large batches and want a repeatable target instead of a feel. The same study let its mixes stand 12 hours before use.

Timing surprise: a wall drying too fast goes chalky-white at the edges within minutes while the middle stays translucent. If you see that edge bloom starting, dampen the surface.

Pigment, Additives, and the Batch-Matching Problem

Weighing pigment for limewash paint test batch colour matching

Pigment is where careful people still ruin a wall. The National Lime Association’s test method is the one to copy: add 1/4 gram of pigment per gallon of limewash, apply it to a 1 sq.ft. Test area, and step up in 1/4-gram increments until you’re happy. Once you land on the dose, scale it proportionally, so 1.25 grams of pigment goes into 5 gallons.

Two things about colour that the sources agree on. Pre-mix pigment with a little hot water before it goes anywhere near the limewash, and expect the finish to turn much lighter as it dries. Colour trials are not optional. They’re the difference between a warm off-white and a wall you’ll be recoating.

Easy to miss: Mix enough limewash to complete a single full coat in one batch. Colour-matching between batches is genuinely difficult, and a half-batch top-up will show as a seam down the middle of the wall.

Additives deserve their own warning. NSW allows an egg-cupful of raw linseed oil if desired, and suggests additives may be better used only in the final coats, if at all. SPAB is colder on the idea: tallow and raw linseed oil both reduce breathability, and tallow may support mould growth without a biocide. The National Park Service notes that historic recipes added tallow during slaking to increase water-shedding, and that it did exactly that while decreasing breathability and making successive layers harder to apply.

If you want the look without the lime chemistry, modern paints built for a limewash effect are a different product with different failure modes. And if you’d rather buy than mix, the best limewash paint shortlist is mostly putty-based products, which is the right instinct.

How Often Does Limewash Need Redoing?

Limewash renewal interval comparison on weathered masonry wall

SPAB says limewash typically requires renewing every five years. The National Park Service says annual reapplication was necessary to counter weathering from exposure. Those are not reconcilable numbers, and anyone who tells you otherwise is quoting one source and ignoring the other.

The variable is exposure. A sheltered internal wall and an exposed exterior wall are not on the same maintenance clock. SPAB’s five-year figure is a typical renewal interval. NPS was writing about cemetery monuments and headstones standing in open weather, which is about as exposed as masonry gets.

There’s a consolation buried in the NPS guidance: successive limewashings require fewer layers. Once the wall has a base, you’re topping up rather than building from scratch.

Skip this if: You want a finish you apply once and forget. Limewash is a sacrificial coating by design. It erodes slowly instead of peeling, which is why it protects the masonry underneath, and it’s also why it comes back on your to-do list.

If your goal is a flat white rather than a lime finish, the process to make whitewash is close but the recipe is not identical, and the limewash vs whitewash distinction matters most when you’re choosing a starting material. Indoors, limewash interior walls follow the same dampening and thin-coat rules, with more attention to airflow while they cure.

Frequently Asked Questions

Can I make limewash with ordinary bagged hydrated lime?

Yes, and both the National Lime Association and NSW give bagged-lime recipes as standard. SPAB cautions that putty made from ordinary non-hydraulic bagged lime can result in inferior limewash, so expect slightly weaker adhesion than a putty-based batch.

How thin should limewash be?

Thin cream, or roughly the consistency of milk. In solids terms that’s about 15 to 20 percent lime and 80 to 85 percent water by weight. If it sits up on the brush instead of flowing off it, add water.

Why did my limewash turn to powder?

Almost always because it dried too fast. The National Park Service explains that rapid drying disrupts carbonation, leaving a weak, cohesionless finish that cracks and powders. Dampen the wall before applying, avoid direct sun and wind, and work in spring or fall.

Do I need to dampen the wall between coats?

Yes. SPAB specifies that each preceding coat should be allowed to dry and the surface dampened down before the next goes on. Skipping it is one of the named causes of poor adhesion.

Can I add linseed oil to make it more weatherproof?

You can, and NSW permits an egg-cupful of raw linseed oil. SPAB counters that linseed and tallow reduce breathability, and that tallow may support mould growth without a biocide. Weigh which property you actually need before adding anything.

How many coats does a first limewashing need?

Three or more, per the National Park Service. SPAB says at least three or four. The first coat on bare masonry is the base for later coats.

Before You Go

The single most useful thing you can do this week is mix a quarter-batch and paint it on a scrap of board you don’t care about. A 1 sq.ft. Patch and 24 hours will tell you more about your particular lime than any ratio table. You’ll see the colour shift as it dries, you’ll feel whether your mix is thin enough, and you’ll find out whether your substrate wants to hold it.

One concession worth stating plainly: everything above assumes a wall that hasn’t been sealed, painted with acrylic, or coated with a water repellent. If yours has, the limewash is not the problem to solve first. Strip the old coating or pick a different wall, because a breathable finish over an impermeable layer does nothing except trap moisture in the masonry where it does the most damage.

And if you’re mixing your first batch and it looks wrong, remember that limewash is semi-transparent going on and only reveals itself once it dries. Make the mark, then keep going.